2311 MOULD STEEL

 

 

STRESS RELIEVING

Heat to 650°C / 750°C.  Hold for 2-4 hours and furnace cool.

 

HARDENING

Before heat treatment, sufficient machining should be carried out to remove
surface decarburisation.
Preheat thoroughly to 650°C / 700°C, and then raise more rapidly to 830°C / 850°C in a controlled atmosphere furnace or preferably, a neutral salt bath.  Quench in oil.