ASP 2005 HIGH-SPEED STEEL

PHYSICAL PROPERTIES
  Temperature °C
20 400 600
DENSITY Kg/m³ 1 7900 7800 7735

MODULUS OF ELASTICITY

kN/mm² 2 220 195 175
COEFFICIENT OF THERMAL EXPANSION FROM  20°C,
per °C
2 - 12.1x10-6 12.7x10-6
THERMAL CONDUCTIVITY W/m °C 2 24 28 27
SPECIFIC HEAT J/kg °C 2 420 510 600
 
1 = Soft annealed
2 = Hardened 1180°C and tempered 560°C, 3x1 hour