ASP 2060 HIGH-SPEED STEEL


 
 
HEAT TREATMENT
  
 

  • Soft-annealing 850°C – 900°C, slow cooling 10°C/h to 700°C, hardness max
    340 HB.
     
  • Stress-relieving annealing 600°C  – 700°C, approx. 2 hours at temperature, slow cooling to 500°C.
     
  • Hardening according to table
    Cooling to 40°C / 50°C.
     
  • Tempering at 560°C 3 times for at least 1 hour each time. Cooling to room temperature (25°C) between temperings.